A stainless bolt fastening a carbon steel bracket is removed months later: a ring of deep pits on the carbon steel, the bolt untouched. The case repeats on outdoor equipment and in wet shops, which sites call a strange phenomenon. It is ordinary galvanic corrosion, with mature countermeasures. The real problem is that design review never treated it as a separate risk.
Three conditions must hold together: a clear difference in corrosion potential, a continuous electrolyte path, and metallic contact for electron flow. Remove any one and the cell stops, which also defines the fix.
Area ratio is underestimated. Current concentrates on the anodic metal, so a small anode against a large cathode gives high current density and rapid loss. A small stainless bolt in a large carbon steel plate is the worst case; reverse it and the carbon steel bolt is consumed quickly.
Carbon steel against 304 or 316 is high risk, with a gap of several hundred millivolts. Carbon steel against zinc plating is moderate, as the zinc sacrifices itself and protects the substrate. Aluminium against stainless is high risk, and pitting once started is hard to stop. Grade 316 resists chloride better than 304, yet sits further from carbon steel, so the driving force is larger.
Insulation is the most effective measure: nylon washers, sleeves or reinforced plastic spacers between the metals, including the shank and the hole wall. Many failures trace back to a bolt touching the bore while washers were correctly fitted. Insulators must resist heat and ageing; polyethylene outdoors fails within a few years.
Next, choose metals close in potential, or make the anode large so the current spreads. A coating works by blocking the electrolyte, but a damaged coating leaves a small anode facing a large cathode and speeds up local attack, so it needs sealing alongside.
Galvanic corrosion is a design issue, not a material defect. Zhuhai Jiali Hardware (FASTKING) supplies stainless, zinc plated and zinc flake fasteners plus insulated washer assemblies. See the screw knowledge section or contact us.